The relationship between blanking gap and shear quality

Source:Suzhou Meiyuan Ruite Precision Machinery Co., Ltd. Time:2022-06-16 Browse:3731


Whether the blanking gap in the blanking process is reasonable will determine whether the upper and lower cracks on the fracture surface overlap, whether the shear force is balanced, and the size of the burr. Therefore, the mold design, manufacture and installation must ensure that the gap is uniform, and the gap between the convex and concave molds in the same manufacturing process should be kept within a reasonable range. Otherwise, the mold will appear part of the gap is too large and too small quality phenomenon.​​
 
Effect of Gap on Section Quality
1. Reasonable blanking gap
When the convex and concave gaps are appropriate, the cracks generated near the edges of the convex and concave die along the direction of the maximum shear stress can meet during the blanking process. At this time, although the section is not perpendicular to the surface of the material, it is still relatively straight, smooth and burr Smaller, the section quality of the part is better.
 
2. Punching gap is too small
When the gap is reduced, the bending moment is small and the compressive stress component is high in the deformation zone. The cracks generated near the edge of the die enter the compressive stress zone below the punch and stop developing; the cracks generated near the edge of the punch enter the compressive stress zone on the upper surface of the die and stop developing. The upper and lower cracks do not overlap. The material between the two cracks will be sheared a second time. When the upper crack is pressed into the die, it is squeezed by the wall of the die, resulting in a second bright band, and at the same time, part of the material is extruded, forming thin and high burrs on the surface. If the gap is too small, although the slump angle is small and the arch is small, the quality of the section is also defective. If there is an interlayer in the middle of the section, the two ends are bright bands, and there are long burrs on the end face.
 
3. Punching gap is too large
When the gap increases, the tensile stress in the material increases, so that the tensile fracture occurs early, so the fracture band becomes wider; the bright band becomes narrower; the bending deformation increases, so the slump and arch also increase. When the gap is too large, due to the large bending moment and the high tensile stress component, the cracks generated near the edges of the convex and concave molds will not coincide. The slope of the fractured layer generated after separation increases, and two oblique angles α1 and α2 appear on the section of the workpiece, and the section quality is not ideal. Moreover, due to the large slump angle, the large arch, the small bright band, and the high and thick burrs, the quality of the blanking parts is reduced.
 
4. The gap is uneven
The side with a small gap presents the cross-sectional feature of an excessively small gap, and the side with a large gap presents the cross-sectional feature of an excessively large gap


主站蜘蛛池模板: 俺去啦最新网址 | 欧美1区| 久久黄色影片 | 99热最新| 国产嫩草影院在线观看 | 又黄又爽又猛大片录像 | 亚洲一级毛片在线观播放 | 福利视频一区二区微拍堂 | 欧美乱妇15p | 久久精品久久久久 | 国产精品成人va在线观看入口 | 欧美一区二区三区在线 | 欧美卡一卡二卡新区网站 | 婷婷99视频精品全部在线观看 | 免费国产不卡午夜福在线观看 | 久久98精品久久久久久婷婷 | 亚洲国产七七久久桃花 | 特黄黄三级视频在线观看 | 国产精品久久久久国产精品三级 | 婷婷综合 在线 | 久久亚洲国产欧洲精品一 | 69色视频| 人人看人人看人做人人模 | 成人综合在线视频 | 天天操91| 欧美色a电影精品aaaa | 国产性夜夜性夜夜爽91 | 亚洲成人三级 | 欧美成人3d动漫在线播放网站 | 国产美女一级ba大片免色 | 好男人社区www在线资源视频 | 欧美不在线| 国产看午夜精品理论片 | 91大神成人偷拍在线观看 | 天天干天天干天天色 | 最近在线观看免费完整视频 | 色偷偷88欧美精品久久久 | 天天视频天天爽 | 久操视频免费看 | 999久久久免费精品国产牛牛 | 亚洲一区二区三区在线视频 |